20

Material:

1.High elasticity and soft hand feeling silicone XG-866NYR+

2.Skin feel matte silicone XG-866M-6+

3.Silicone catalyst XG-866B-2

4.Fluorescent orange pigment XG-134

5.Silicone thinner XG-128AH

6.Screen:1 pcs,40T mesh

7.Squeegee:70 ShoreA

 

Printing process

1.Based coating:use XG-866NYR+ with 2% XG-866B-2,10% XG-128AH to print 4-6 times(two strikes each time,120-150℃ to bake ink to dry than go on)

2.Orange color printing:use XG-866NYR+ with 2% XG-866B-2,10% XG-128AH,10% XG-134 to print 2-4 times(two strikes each time,120-150℃ to bake ink to dry than go on)

3.Top coating:use skin feel matte silicone XG-866M-6+ with 2% XG-866B-2 to print 2 times(two strikes each time,120-150℃ to bake ink to dry)